Sep 26, 2025 Leave a message

An Innovative Safe Process for Producing MgFeSi Alloy Containing Calcium and Rare Earth Elements

Abstract

Magnesium has long been used to improve the mechanical properties of cast iron. It is currently added to ductile iron during production in the form of a magnesium-ferrosilicon (MgFeSi) alloy. Numerous methods exist for producing MgFeSi alloys, most of which employ dolomite reduction or ferrosilicon-magnesium remelting. However, these methods present technical challenges, in addition to low magnesium recovery rates. This study developed a novel process for producing MgFeSi alloys by coating the magnesium ingot with a flux protective layer to slow the reaction between magnesium and liquid ferrosilicon, reduce magnesium oxidation, and thus improve magnesium recovery. This innovative process has proven to be highly effective, achieving a magnesium recovery rate of 87.35% and a rare earth element recovery rate of 99.59%. It safely produces a MgFeSi alloy containing 9.58% Mg, 1.26% rare earth elements (REEs), and 1.52% Ca by weight.

 

Introduce

Magnesium-iron-silicon alloy (MgFeSi) is commonly used in the iron casting industry as an essential additive in the production of ductile iron to promote the dispersion and formation of spherical graphite, or graphite nodules, within the matrix. This graphite shape imparts excellent ductility to the material, resulting in a material that combines good ductility with high strength, good machinability, and a smooth surface finish.

With the discovery of spheroidal graphite structures, the use of magnesium to form spheroidal graphite within an iron matrix was proposed and tested as a replacement for traditional flake graphite. Although magnesium is highly effective as a nodularizing agent, its low density (1.74 gm cm −3 ), low boiling point (1107°C), limited solubility in cast iron, and high vapor pressure at ductile iron production temperatures make it difficult to use pure magnesium. The addition of magnesium also results in a violent reaction, causing intense agitation of the molten iron and the generation of white magnesium oxide fumes, resulting in magnesium loss and reduced magnesium recovery.

Research has found that magnesium dissolves in molten ferrosilicon alloys to form stable magnesium silicide. The resulting MgFeSi alloy has a higher density than pure magnesium metal and is considered an excellent alloy for introducing magnesium into molten cast iron. To form magnesium silicide and reduce the severity of the reaction, the optimal silicon content in ferrosilicon-magnesium alloys is 40% to 50%, while the magnesium content is typically between 5% and 10%.

Later research demonstrated that calcium can form spherical graphite and reduce magnesium loss. Adding calcium to ferrosilicon-magnesium alloys introduces a second magnesium-containing phase, CaMgSi2, into the structure , reducing the reaction rate and thus positively impacting magnesium recovery. Rare earth elements also demonstrated the ability to form spherical structures, and cerium (Ce) and lanthanum (La) were subsequently introduced into the production of ferrosilicon-magnesium alloys.

Magnesium-containing ferrosilicon alloys can be produced by reducing magnesium-containing ores (such as dolomite) with carbon, silicon, or aluminum. However, using carbon as a reducing agent in an electric arc furnace to produce magnesium-containing ferrosilicon alloys presents significant challenges due to the high operating temperature and vapor pressure of magnesium. Furthermore, the high cost of using aluminum in the production process and the high aluminum content of the resulting alloy make this process less than ideal. Furthermore, magnesium recovery rates do not exceed 13.8% when reducing calcined dolomite ore with silicon or silicon-aluminum reduction.

In addition to the reduction process, magnesium-iron silicon alloys with a magnesium content of about 5.5% can also be produced by immersing magnesium ingots in molten ferrosilicon. The immersion method is more economical than the reduction method, but it has technical challenges. Magnesium reacts with molten ferrosilicon, generating high heat, sparks, smoke and fumes. The magnesium content and magnesium recovery rate of the alloy are also low. In another study, researchers conducted laboratory experiments to immerse magnesium in ferrosilicon melt to reduce the severity of the reaction and increase the silicon content to as high as 75%. However, the maximum magnesium recovery rate was only 71%, and the magnesium content in the final alloy did not exceed 9.5%. In addition, the MgFeSi alloy produced has a high silicon content of 65–75%. , which is not suitable for producing ductile iron castings. Another technique is to melt magnesium silicide and ferrosilicon together to produce magnesium-ferrosilicon alloy. Experiments were conducted in the laboratory. This method requires melting under an inert gas atmosphere and using pressures above atmospheric pressure to reduce magnesium oxidation. Another method for producing magnesium-ferrosilicon alloy is to remelt the magnesium while protecting it from oxidation with slag. Solid ferrosilicon is slowly added to the melt as the temperature gradually increases. This process follows the silicon-magnesium relationship diagram to maintain fluidity and keep the metal in a liquid state. This method is complex and requires a careful balance between the amount of ferrosilicon added and the temperature increase. Because large amounts of ferrosilicon must be added slowly, the heating time is prolonged, resulting in low productivity.

In summary, all different methods for producing magnesium-iron-silicon alloys face challenges, particularly low magnesium recovery rates. Magnesium is the most expensive raw material in the process, leading to increased production costs and negatively impacting the economics of the production process. Therefore, further research is needed to find a safer method for producing ferrosilicon-magnesium alloys with higher magnesium recovery rates.

This study aims to explore a method for safely producing silicon-magnesium-iron alloys containing rare earth elements and with high magnesium recovery.

 

Experiment

To determine the optimal conditions for producing ferrosilicon-magnesium alloys with high magnesium content and maximum magnesium recovery, pilot furnace trials were designed and conducted at the China Metallurgical Research and Design Institute's Iron and Steel and Ferroalloy Pilot Facility (Pilot Facility). The trials utilized an electric arc furnace and various casting processes. The raw materials required for the pilot trials were identified and included ferrosilicon alloy, steel scrap, magnesium ingots, calcium-silicon alloy, rare earth elements, flux, and coating materials (ferrosilicon powder, dolomite, talc, and boric acid). X-ray and wet chemical analysis were performed on the various raw materials.

 

The magnesium ingot used contains 99% Mg and the boric acid contains 99.9 % H3BO3

Based on chemical analysis of the various raw materials, a material balance was performed to produce an MgFeSi alloy containing 40–46% Si, 9–11% Mg, 1–1.5% Ca, and 1.25–1.5% REEs (Ce and La). The required amounts of the various raw materials were determined based on the material balance. 5.1–5.65 kg of magnesium ingot was added to produce an MgFeSi alloy containing 9–11% Mg. The raw materials used to coat the magnesium ingot (ferrosilicon powder, dolomite, talc, and boric acid) had a particle size of less than 3 mm. The various components of the magnesium surface coating were thoroughly mixed in a blender, and then a simple coating was applied to 90% of the ingot surface using sodium silicate as a binder.

Seven pilot experiments were conducted to produce magnesium-ferrosilicon alloys containing calcium and rare earth elements. Molten ferrosilicon was produced using a 100 kVA electric arc furnace. In these experiments, the charge consisted of either 40 kg of ferrosilicon alloy and 15 kg of scrap steel or 41.5 kg of ferrosilicon alloy and 13.5 kg of scrap steel to reduce the silicon content and increase the iron content, thereby obtaining a ferrosilicon melt with the desired silicon content. The optimum silicon content for ferrosilicon-magnesium alloys is 40% to 50% to facilitate the formation of magnesium silicides and reduce the severity of the reaction. After complete melting at 1600°C, the molten metal was poured into a hot ladle containing calcium silicon, rare earth elements, and magnesium ingots. Figure 1 shows a schematic diagram of the casting process for producing the MgFeSi alloy. Magnesium ingots coated with a flux shield or uncoated with rare earth metals were placed at the bottom of the hot ladle, covered with calcium silicon, and then poured with molten FeSi, as shown in Figure 1. In one experiment (Group 1), uncoated magnesium ingots were used. In the other experiments, 90% The surface of magnesium ingots was coated with FeSi fine powder or a mixture of different fluxes and coating materials with sodium silicate as a binder to study the effect of the coating process on magnesium recovery. Additives were selected to promote endothermic reactions in the melt, thereby reducing the temperature. 

 

After tapping, the melting of the various components and their reaction with the molten ferrosilicon are complete within 2-3 minutes. The resulting metal is weighed, and a representative alloy sample is taken for XRF chemical analysis. XRD analysis is also performed on the resulting alloy sample.

 

Figure 1

 ​

Figure 1

​

 

 

The magnesium recovery results demonstrate the effectiveness of the innovative process in improving magnesium recovery in magnesium-ferro-silicon alloy production. When molten ferrosilicon was poured into a ladle containing calcium silicon, rare earth elements, and uncoated magnesium ingots, magnesium recovery was low at 69.49%. By coating 90% of the magnesium ingot surface with ferrosilicon powder equivalent to 44% of the ingot weight, magnesium recovery was increased to 84.96%. By coating 90% of the magnesium ingot surface with a protective layer consisting of a mixture of dolomite, talc, and boric acid, or dolomite, talc, boric acid, and ferrosilicon powder, magnesium recovery was increased to 85.11% to 87.35%. The highest magnesium recovery (87.35%) was achieved by coating 90% of the magnesium ingot surface with a protective layer composed of a mixed flux material comprising 29% of the ingot weight, including 36.5% dolomite, 36.5% ferrosilicon powder, 24% talc, and 3% In addition to the protective layer's strengthening effect, the calcium-silicon alloy also appears to improve magnesium recovery. The magnesium recovery rate for the second heat (84.00%), without the addition of calcium-silicon alloy, was lower than the magnesium recovery rate for the seventh heat (87.35%), produced under the same conditions but with the addition of calcium-silicon. This higher magnesium recovery resulted in a higher magnesium content in the produced MgFeSi alloy, ranging from 9.04% to 10.89%.

 

Furthermore, by coating 90% of the magnesium ingot surface with a protective layer, the recovery of total rare earth elements (Ce+La) increased from 88.7% when using uncoated magnesium ingots to higher values ​​of 95.26–99.59%.

 

Compared to the much lower magnesium recovery rates (no more than 13.8%) achieved when reducing Cabernet dolomite with silicon or alumina, or the maximum magnesium recovery of 71% achieved when magnesium was leached into ferrosilicon melts, the significantly higher magnesium recovery rate in this study (87.35%) can be attributed to several factors. When pouring molten ferrosilicon onto an uncoated magnesium ingot, magnesium reacts vigorously due to its low density, low boiling point, and high vapor pressure at molten ferrosilicon temperatures, resulting in significant magnesium evaporation. Furthermore, without slag covering the molten metal surface, magnesium oxidizes, leading to low magnesium recovery.

 

By coating 90% of the magnesium ingot's surface, the remaining uncoated magnesium begins to react, and the coating plays a major role in reducing magnesium loss. If ferrosilicon powder is coated on the surface of the magnesium ingot, its melting is an endothermic process, absorbing heat and thus lowering the molten pool temperature, slowing the magnesium reaction and minimizing magnesium loss due to evaporation.

In addition to its positive effect on the other components of the mixture (dolomite, talc, and boric acid), the protective layer of ferrosilicon powder has other effects. The decomposition of dolomite and talc ore is an endothermic reaction that reduces the temperature of the molten pool. Boric acid loses all water above 150°C and is converted into boron oxide (B2O3 ) , which acts as a flux and lowers the melting point of the different oxides of talc and dolomite, thereby increasing the fluidity of the slag formed by these oxides. The resulting fluid slag has a lower density than the molten metal and floats on the surface of the molten metal, forming an effective protective layer that prevents atmospheric oxygen from penetrating into the molten metal and reduces the oxidation of magnesium. This slag layer also prevents any magnesium vapor that may form from escaping into the air. As a result, any magnesium vapor that may form has time to react with silicon and calcium to form magnesium silicide and calcium magnesium silicide. XRD analysis of the resulting magnesium-iron-silicon alloy revealed the formation of magnesium silicide ( Mg2 The formed magnesium silicide and calcium magnesium silicide intermetallic phases reduce the vapor partial pressure of magnesium in the molten metal.

 

In addition, the small amount of magnesium oxide in talc and dolomite may be partially reduced to Mg, or magnesium silicide may enter the resulting alloy phase, thereby improving the magnesium recovery rate. The presence of CaO makes it easier for MgO to be reduced to Mg2Si , and the reduction temperature can reach 1650-1750℃.

 

In conclusion

For the production of magnesium-silicon-iron alloys containing calcium and rare earth elements, coating a flux protective layer on the surface of the magnesium ingot can effectively improve the magnesium recovery rate.

By coating 90% of the magnesium ingot surface with ferrosilicon fine powder equivalent to 44% of the ingot weight, the magnesium recovery rate increased from 69.49% to 84.96%.

 

Higher magnesium recoveries of 85.11–87.35% were achieved by coating 90% of the magnesium ingot surface with a protective layer consisting of a mixture of dolomite, talc, and boric acid or dolomite, talc, boric acid, and ferrosilicon powder.

In addition to enhancing the protective layer, the calcium-silicon alloy also appears to help improve magnesium recovery.

 

The highest magnesium recovery (87.35%) was achieved by coating 90% of the magnesium ingot surface with a protective layer of mixed flux material. This protective layer, which accounts for 29% of the ingot weight, consists of 36.5% dolomite, 36.5% ferrosilicon powder, 24% talc, and 3% boric acid.

In addition to higher magnesium recovery, the total rare earth element (Ce+La) recovery rate was also increased from 88.7% to 95.26-99.59% by using uncoated magnesium ingots (by applying a protective coating on 90% of the magnesium ingot surface).

 

The high magnesium recovery rate results in a high magnesium content in the produced MgFeSi alloy, ranging from 9.04% to 10.89%. Under optimal protection conditions, a ferrosilicon-magnesium alloy containing 9.58% magnesium, 1.26% rare earth elements, and 1.52% calcium can be safely obtained.

 

Send Inquiry